Technical Articles
CFRP/Titanium Stack Drilling: Choose the Drill for the Whole Hole
A drill sails through CFRP coupon tests, then goes into a CFRP/titanium stack and the composite bore comes out scored and heat-damaged after the cutting edges have already passed through it. That's not bad luck. In a CFRP-first stack, drilling the titanium can damage the CFRP you just cut, so a single-material result can't pick your tool. Here's how to define the hole, understand the damage mechanism, and run a trial that judges the complete stack and its hidden interface.

Contents
Define the hole before you compare drills
Spell out the drilling direction: entry side, layer order and final exit side. A label like "CFRP/Ti" only works if everyone reads it the same way. Then nail down the actual laminate and titanium grade, each layer's thickness, the interface condition, and the support and clamping setup. These define the application you're selecting for. They aren't details to fill in after someone has already picked a point angle.

For background on the individual materials, see our CFRP material background and titanium machining considerations. Neither replaces stack-specific tool and process evidence.
Next, split the quality requirements by location. Pull the limits from your drawing and process specification, not from a research paper.
| Location to distinguish | What the comparison needs to reveal | What a single good-looking result can miss |
|---|---|---|
| CFRP layer | Fiber damage, delamination and signs of thermal or abrasive damage at the relevant faces and bore surface | A clean entry face can hide damage deeper in the hole or at the interface. |
| Titanium layer | Burrs at its entry and exit, plus the specified bore dimensions and surface condition | A small burr tells you nothing about diameter or surface finish. |
| Internal material interface | Damage on the mating faces, plus any interlayer burr or chip ingress | The outside faces don't show what happened between the layers. |
| Hole through the assembly | The required dimensional relationship through the full stack, checked with a suitable inspection method | A good result in one layer says nothing about the other. |
In a CFRP-entry, titanium-below stack, the CFRP layer exits at the internal interface. The titanium exit is the final exit of the stack. Lump both under "exit quality" and you lose the location you need to diagnose the defect.

Match the inspection method to the material, too. Protruding fibers can throw off a composite bore measurement, so don't assume a gauging routine that works on titanium describes the CFRP surface just as well. Lock the method before comparing tools, or a change in measurement will masquerade as a change in performance.
Why the CFRP gets damaged after it's already cut
At the material transition, different parts of the cutting edges can be engaged in both materials at once. Later, with the drill point in titanium, the composite bore you already cut is still part of the tool and chip path. This is not two independent single-material holes.
Andrea Pardo and coauthors' study of interface borehole quality looked at conventional drilling with CFRP as the entry layer and titanium underneath. The researchers attributed much of the CFRP interface damage to the titanium-cutting stage that came after. Hot titanium chips traveling up the flutes abraded the composite and transferred heat into it. Heat buildup near the interface and heat conducted through the tool were also flagged as damage mechanisms.

Some titanium chips also forced their way into the gap between layers. In controlled-gap tests, a wider interlayer gap made chip ingress easier and increased damage to the CFRP interface surface. So if damage persists after a drill change, look hard at the actual interface and the fixture. Just don't expect every defect to move the same way: the researchers found no clear monotonic relationship between gap width and the height of the titanium entry interlayer burr.

Drilling order matters as well. Putting titanium first changes where the titanium chips go, but it also changes the support under the CFRP as the drill breaks out of that layer. Reversing the stack is a different process condition to evaluate, not a cure-all for composite damage. Keep any backing arrangement in that comparison.
Compare the full geometry, then read force alongside hole quality
Point geometry controls how the cutting edges engage the interface and how titanium chips form and travel through the flutes. Improve one of those behaviors and you can make another worse. In Pardo's tests, the smallest point angle did not produce the least CFRP interface damage. Chip flow, torque and heat explain why the trend from single-layer CFRP drilling broke down in the stack.
Don't read that as a new "best" angle. The tested drills also differed in details such as faceting and notches; they weren't identical tools with one number changed. When you compare candidates, keep the complete geometry on record: point and chisel region, flute design and edge condition. A nominal point angle alone can't account for everything behind a result.
Treat force data the same way. Lower thrust can matter for composite damage, but a force reading is not a hole inspection. It won't report titanium burrs, bore size, surface damage or the condition of the hidden interface. In the cited study, unstable chip flow and torque fluctuations helped explain poor surface results that an angle-only comparison would have missed.
If you have force and torque data, tie it to the cutting stage and to the defects at the matching location. A whole-cycle peak can hide whether the disturbance happened in the CFRP, at the transition or in the titanium. Use the signals to investigate a result, always next to the actual hole measurements.

Design a trial that exposes a misleading winner
A useful stack-drilling trial has to catch the drill that looks great on one metric and fails somewhere else. Before you run it:
Set the required quality checks for each material, the internal interface and the final stack exit. Decide how hidden interface damage will be examined on the trial samples.
Record the actual stack, fixture, interface condition, tool geometry and drilling cycle. Keep the coolant method and the tool's prior use attached to the results.
Judge repeated holes, not the best photo. Pardo's team saw substantial interface-quality differences between holes drilled under nominally identical conditions, linked to variation in chip flow and chip jamming.
Keep chip observations and any stage-resolved force or torque data next to the location-specific inspection results. If one outcome improves while another gets worse, record that tradeoff instead of collapsing the trial into a single score.


Keep geometry screening and tool-life testing separate. The cited geometry study deliberately limited tool wear during its comparison. A test like that shows you useful cutting behavior; it can't tell you how long that behavior lasts in production. Tool-life evaluation needs the hole sequence and tool condition recorded, with the applicable quality checks and agreed wear limits applied as usage builds up.

When you take results to a tool supplier, bring the layer materials and layup, thicknesses and order, interface and backing conditions, hole requirements, machine and coolant method, and evidence of each defect at its actual location. Ask what stack-specific trial evidence backs the proposed drill. A good single-material result opens the conversation. The final call belongs to the finished hole in the specified assembly.